Plastic shrinkage rate guide: Injection molding shrink rates by material

Rosti Poland design team

Plastic material shrinkage refers to the reduction in size of a molded part as it cools after injection. Every material has a different shrink rate, which depends on the resin family (amorphous vs. crystalline materials), mold design, and processing conditions.

Understanding material shrinkage is crucial for achieving dimensional accuracy, minimizing warpage, and preventing part failure in injection molded components. This Molding Material Shrink Rate Guide provides typical mold shrink rates, tonnage recommendations, and vent depth values for a selection of commonly used materials and high-heat resins.

The complete shrinkage chart is shown below, and you can download the full PDF guide using the whitepaper button above for quick reference.

What is shrinkage in injection molding?

Mold shrinkage is the reduction in size of a molded part as it cools from a molten state to room temperature. Shrinkage rates are usually expressed as in/in (or mm/mm) and may also be shown as a percentage. For example, .004 – .008 in/in is equal to 0.4 – 0.8% shrinkage. The chart below lists shrinkage values in in/in (as used in the downloadable PDF), while percentage equivalents are provided throughout this guide to make it easier to compare materials, since many engineers and designers search for shrinkage data by percentage.

Why do plastics shrink?

Plastic material shrinkage starts at the molecular level as the polymer cools from a molten state to room temperature. As the material loses heat, its molecules move closer together, which causes the molded part to contract. The amount of contraction depends mainly on the polymer’s molecular structure, making material selection a key factor in achieving dimensional accuracy.

The largest distinction is between amorphous and semi-crystalline thermoplastics:

  • Amorphous materials – such as ABS, Polycarbonate (PC), Polystyrene (PS), and Acrylic (PMMA) have randomly arranged molecular chains. Since they don’t form crystalline regions during cooling, they usually have lower and more consistent shrinkage, making it easier to mold them to tight tolerances.
  • Semi-crystalline materials – including HDPE, Polypropylene (PP), Acetal (POM), and Nylon (PA), develop ordered crystalline structures as they cool. This crystallization packs the polymer chains more tightly, causing higher shrinkage rates and a greater risk of uneven shrinkage and warpage if the mold and process aren’t carefully controlled.

Shrinkage is also directional. Plastic tends to shrink differently in the direction of melt flow than across the flow, especially in semi-crystalline and fiber-reinforced materials. Designers and mold makers need to take both flow and crossflow shrinkage into account when setting cavity dimensions and predicting part distortion.

Another important factor is the use of fillers and fiber reinforcement. Glass fibers and mineral fillers reduce overall shrinkage by limiting polymer movement during cooling, and they also make shrinkage more uniform. This effect is clear in the guide’s shrinkage data for nylon:

  • Polyamide (Nylon) Filled – .005 -.010 in/in (0.5 – 1.0%)
  • Polyamide (Nylon) Unfilled – .007 -.025 in/in (0.7 – 2.5%)

The much lower shrinkage range of filled nylon shows how reinforcement can improve dimensional stability and reduce the risk of warpage, making it a preferred material for precision engineering applications requiring tight tolerances.

Mold shrinkage chart – shrink rates by material

MaterialRecommended Tonnage (per in2)Shrink ValuesVent depth (in.)
Acrylonitrile Butadiene Styrene (ABS)2.5 – 3.5.004 – .008.0010 – .0020
ABS/Polycarbonate Blend (PC/ABS)3.0 – 4.0.004 – .007.0015 – .0030
Acetal (POM)3.0 – 4.0.020 – .035.0005 – .0015
Acrylic (PMMA)3.0 – 4.0.002 – .010.0015 – .0020
Ethylene Vinyl Acetate (EVA)2.0 – 3.0.010 – .030.0005 – .0007
Ionomer2.5 – 3.5.003 – .020.0005 – .0007
High Density Polyethylene (HDPE)2.5 – 3.5.015 – .030.0008 – .0010
Low Density Polyethylene (LDPE)2.0 – 3.0.015 – .035.0005 – .0007
Polyamide – Nylon (PA) Filled4.0 – 5.0.005 – .010.0003 – .0010
Polyamide – Nylon (PA) Unfilled3.0 – 4.0.007 – .025.0005 – .0020
Polybutylene Terephthalate (PBT)3.0 – 4.0.008 – .010.0005 – .0015
Polycarbonate (PC)4.0 – 5.0.005 – .007.0010 – .0030
Polyester2.5 – 3.5.006 – .022.0005 – .0010
Polyetheretherketone (PEEK)4.0 – 5.0.010 – .020.0005 – .0007
Polyetherimide (PEI)3.0 – 4.0.005 – .007.0010 – .0015
Polyethylene (PE)2.5 – 3.5.015 – .035.0005 – .0020
Polyethersulfone (PES)3.0 – 4.0.002 – .007.0005 – .0007
Polyphenylene Oxide (PPO)3.0 – 4.0.005 – .007.0010 – .0020
Polyphenylene Sulfide (PPS)3.5 – 4.5.002 – .005.0005 – .0010
Polyphthalamide (PPA)3.5 – 4.5.005 – .007.0005 – .0020
Polypropylene (PP)2.5 – 3.5.010 – .030.0005 – .0020
Polystyrene (PS)2.0 – 2.5.002 – .008.0015 – .0020
Polysulphone (PSU)4.0 – 5.0.006 – .008.0010 – .0015
Polyurethane (PUR)2.5 – 3.5.010 – .020.0004 – .0010
Polyvinyl Chloride (PVC)2.5 – 3.5.002 – .030.0005 – .0020
Thermoplastic Elastomer (TPE)2.5 – 3.5.005 – .020.0008 – .0010

Shrink rates for common materials

HDPE Shrink Rate

HDPE shrink rate – .015–.030 in/in (1.5 – 3.0%). High Density Polyethylene (HDPE) is a semi-crystalline thermoplastic, which gives it one of the highest shrinkage ranges typically seen in injection molding. As the polymer crystallizes during cooling, its molecular structure becomes more tightly packed, leading to greater contraction than amorphous plastics. For HDPE shrinkage in injection molding, mold cavity sizing, uniform wall thickness, consistent cooling, and generous draft angles are essential to minimize warpage and maintain dimensional accuracy.

ABS Shrink Rate

ABS shrinkage rate  .004- .008 in/in (0.4 – 0.8%). As an amorphous thermoplastic, ABS has relatively low and predictable shrinkage because it doesn’t crystallize during cooling. This makes it a popular choice for parts that require tight tolerances and good dimensional stability. For comparison, PC/ABS blends have a slightly lower shrinkage range of .004 – .007 in/in (0.4 – 0.7%), providing even greater dimensional consistency while combining the toughness of polycarbonate with the processability of ABS.

Polypropylene Shrink Rate

Polypropylene (PP) shrinkage rate   .010 – .030 in/in (1.0 – 3.0%). PP is a semi-crystalline resin with relatively high and variable shrinkage due to crystallization during cooling. The final shrinkage can vary a lot depending on part geometry, wall thickness, mold temperature, and cooling conditions. Designers should account for this variability early in the tool design process by using uniform wall sections and balanced cooling to help reduce differential shrinkage, sink marks, and warpage.

Nylon Shrinkage

Nylon (Polyamide) shrinkage varies widely depending on whether or not the material is reinforced. Unfilled nylon usually shrinks .007 – .025 in/in (0.7 – 2.5%), while glass-filled nylon shrinks only .005 – .010 in/in (0.5 – 1.0%). Glass fibers limit polymer movement as the material cools, which reduces overall shrinkage and makes it more uniform. This improved dimensional stability is a primary reason why glass-filled nylon is used for precision engineering components that require tight tolerances and minimal warpage.

How to calculate shrinkage percentage

Plastic shrinkage is typically calculated using the following formula:

Shrinkage (%) = (Mold cavity dimension − Finished part dimension) ÷ Mold cavity dimension × 100

Worked Example

If a mold cavity is 100.0 mm long and the finished molded part measures 99.3 mm, the shrinkage is:

Shrinkage (%) = (100.0 − 99.3) ÷ 100.0 × 100 = 0.7%

This is equivalent to a shrinkage rate of .007 in/in (0.007 mm/mm).

How Toolmakers Use the Shrink Factor

Toolmakers account for material shrinkage before the mold is manufactured by cutting the mold cavity oversize. The cavity dimensions are increased by the expected shrink factor so that, after the molten plastic cools and contracts, the finished part reaches its required dimensions.

For example, if a component must measure 100.0 mm after molding and the selected material has a shrinkage rate of 0.7% (.007 in/in), the mold cavity would be machined to approximately 100.7 mm. As the part cools and shrinks by around 0.7 mm, it produces a finished component close to the target 100.0 mm dimension. Because actual shrinkage is also influenced by part geometry, wall thickness, mold design and processing conditions, toolmakers often fine-tune cavity dimensions during tool trials to achieve the final required tolerances.

What affects the shrinkage rate?

Although every material has a typical shrinkage range, the actual amount of shrinkage depends on both the resin and the molding process. Key factors include:

  • Mold temperature – Mold temperature has a significant influence on shrinkage. As a general guide, a 10% change in mold temperature can result in approximately a 5% change in the original shrinkage rate, particularly for semi-crystalline materials.
  • Injection pressure – Higher injection pressure packs more material into the cavity, increasing density and generally reducing shrinkage. Lower packing pressure typically results in greater shrinkage.
  • Resin family and fillers – Amorphous resins generally shrink less than semi-crystalline resins, while glass fiber and mineral-filled grades reduce shrinkage and improve dimensional stability compared with unfilled materials.
  • Flow direction – Shrinkage is often different parallel to the melt flow than across the flow, especially in semi-crystalline and fiber-reinforced materials, and should be considered during tool design.
  • Wall thickness – Thicker sections cool more slowly and tend to shrink more than thin, uniform walls, increasing the risk of sink marks and warpage.
  • Cooling time – Consistent and adequate cooling promotes more uniform shrinkage, while uneven cooling can lead to distortion and dimensional variation.
  • Gate location – Gate position influences material flow, packing pressure and cooling patterns, all of which affect shrinkage distribution and the likelihood of warpage across the finished part.

What is an acceptable shrinkage percentage?

There is no universal “acceptable” plastic shrinkage percentage. What is acceptable depends on the dimensional tolerance, function and performance requirements of the finished part—not the shrinkage value itself. Materials with low shrinkage, such as amorphous resins, are often selected for precision components because they are easier to mold to tight tolerances. Typical shrinkage ranges from 0.2 – 0.8%, depending on the material. In contrast, semi-crystalline resins commonly shrink 1.5 – 3.5%, but these higher values are entirely acceptable when the mold is designed with the correct shrink allowance and the process is properly controlled. The key is not achieving the lowest possible shrinkage but accurately compensating for the material’s expected shrinkage during tool design to produce parts within specification.

How Rosti compensates for shrinkage in mold design

At Rosti, plastic shrinkage is considered from the earliest stages of product development to ensure components meet their dimensional and performance requirements. Our engineering teams account for shrinkage throughout the development process in three key stages:

  • Material selection – Selecting the most appropriate polymer based on shrinkage characteristics, mechanical performance and dimensional stability.
  • Mold flow simulation – Using mold flow analysis to predict material flow, packing, cooling and expected shrinkage before tooling is manufactured, helping to reduce development risk and optimize part quality.
  • Tool design and validation – Applying the correct shrink factors when designing and machining the mold cavity, then validating dimensions during tool trials to achieve the required tolerances.

Learn more about our Material Selection, Mold Flow Simulation, Tool Design & Validation capabilities to see how we engineer high-quality injection molded components from concept through production.

If you’re developing a new injection molded component or selecting the right material for your application, contact Rosti’s engineering team to discuss your design, tooling and manufacturing requirements.

FAQ

Why does polypropylene shrink more than ABS?

Polypropylene (PP) typically shrinks 1.0 – 3.0%, compared to 0.4 – 0.8% for ABS. This difference comes from their molecular structure: PP is semi-crystalline, so its polymer chains pack more tightly as they crystallize while cooling. ABS is amorphous, which means it cools without crystallization and thus contracts less and more evenly.