Plastic shrinkage rate guide: Injection moulding shrink rates by material

Plastic material shrinkage occurs in the contraction of a moulded part as it cools after injection. All materials have different shrink rates depending on resin family (amorphous vs. crystalline materials) mould design and processing conditions. Understanding material shrinkage is critical for achieving dimensional accuracy, minimising warpage and preventing part failure in injection moulded components.

This Moulding Material Shrink Rate Guide outlines typical mould shrink rates, as well as tonnage recommendations and vent depth values, for some common to moderately used materials and high heat resins. The full shrinkage chart is provided below, and you can download the complete PDF guide using the whitepaper button above for quick reference.

What is shrinkage in injection moulding?

Mould shrinkage is the contraction of a moulded part as it cools from the molten state to ambient temperature. Shrinkage rates are commonly expressed as in/in (or mm/mm) and can also be shown as a percentage. For example, .004 – .008 in/in is equivalent to 0.4 – 0.8% shrinkage.

The chart below presents shrinkage values in in/in (as used in the downloadable PDF) while the equivalent percentage values are also provided throughout this guide to make comparing materials easier, since many engineers and designers search for shrinkage data as percentages.

Why do plastics shrink?

Plastic material shrinkage begins at the molecular level as the polymer cools from the molten state to room temperature. As the material loses heat, its molecules move closer together, causing the moulded part to contract. The amount of contraction depends largely on the polymer’s molecular structure, making material selection a key factor in achieving dimensional accuracy.

The biggest distinction is between amorphous and semi-crystalline thermoplastics:

  • Amorphous materials – such as ABS, Polycarbonate (PC), Polystyrene (PS), and Acrylic (PMMA) have randomly arranged molecular chains. Because they do not form crystalline regions during cooling, they typically exhibit lower and more uniform shrinkage, making them easier to mould to tight dimensional tolerances. 
  • Semi-crystalline materials – including HDPE, Polypropylene (PP), Acetal (POM), and Nylon (PA) develop ordered crystalline structures as they cool. This crystallisation packs the polymer chains more tightly, resulting in higher shrinkage rates and a greater likelihood of differential shrinkage and warpage if the mould and process are not carefully controlled. 

Shrinkage is also directional. Plastic tends to shrink differently in the direction of melt flow than across the flow, particularly in semi-crystalline and fiber-reinforced materials. Designers and mould makers must account for both flow and cross-flow shrinkage when determining cavity dimensions and predicting part distortion.

Another important factor is the use of fillers and fiber reinforcement. Glass fibers and mineral fillers reduce overall shrinkage by restricting polymer movement during cooling, while also making shrinkage more uniform. This effect is evident in the guide’s shrinkage data for nylon:

  • Polyamide (Nylon) Filled – .005 -.010 in/in (0.5 – 1.0%) 
  • Polyamide (Nylon) Unfilled – .007 -.025 in/in (0.7 – 2.5%) 

The significantly lower shrinkage range of filled nylon demonstrates how reinforcement can improve dimensional stability and reduce the risk of warpage, making it a preferred choice for precision engineering applications where tight tolerances are required.

Mould shrinkage chart – shrink rates by material

Typical mould shrink rates, recommended tonnage, and vent depth by material.
Material Recommended tonnage (per in²) Shrink values (in/in) Vent depth (in.)
Acrylonitrile Butadiene Styrene (ABS)2.5 – 3.5.004 – .008.0010 – .0020
ABS/Polycarbonate Blend (PC/ABS)3.0 – 4.0.004 – .007.0015 – .0030
Acetal (POM)3.0 – 4.0.020 – .035.0005 – .0015
Acrylic (PMMA)3.0 – 4.0.002 – .010.0015 – .0020
Ethylene Vinyl Acetate (EVA)2.0 – 3.0.010 – .030.0005 – .0007
Ionomer2.5 – 3.5.003 – .020.0005 – .0007
High Density Polyethylene (HDPE)2.5 – 3.5.015 – .030.0008 – .0010
Low Density Polyethylene (LDPE)2.0 – 3.0.015 – .035.0005 – .0007
Polyamide – Nylon (PA), filled4.0 – 5.0.005 – .010.0003 – .0010
Polyamide – Nylon (PA), unfilled3.0 – 4.0.007 – .025.0005 – .0020
Polybutylene Terephthalate (PBT)3.0 – 4.0.008 – .010.0005 – .0015
Polycarbonate (PC)4.0 – 5.0.005 – .007.0010 – .0030
Polyester2.5 – 3.5.006 – .022.0005 – .0010
Polyetheretherketone (PEEK)4.0 – 5.0.010 – .020.0005 – .0007
Polyetherimide (PEI)3.0 – 4.0.005 – .007.0010 – .0015
Polyethylene (PE)2.5 – 3.5.015 – .035.0005 – .0020
Polyethersulfone (PES)3.0 – 4.0.002 – .007.0005 – .0007
Polyphenylene Oxide (PPO)3.0 – 4.0.005 – .007.0010 – .0020
Polyphenylene Sulfide (PPS)3.5 – 4.5.002 – .005.0005 – .0010
Polyphthalamide (PPA)3.5 – 4.5.005 – .007.0005 – .0020
Polypropylene (PP)2.5 – 3.5.010 – .030.0005 – .0020
Polystyrene (PS)2.0 – 2.5.002 – .008.0015 – .0020
Polysulphone (PSU)4.0 – 5.0.006 – .008.0010 – .0015
Polyurethane (PUR)2.5 – 3.5.010 – .020.0004 – .0010
Polyvinyl Chloride (PVC)2.5 – 3.5.002 – .030.0005 – .0020
Thermoplastic Elastomer (TPE)2.5 – 3.5.005 – .020.0008 – .0010

Shrink rates for common materials

HDPE Shrink rate

HDPE shrink rate – .015–.030 in/in (1.5 – 3.0%). High Density Polyethylene (HDPE) is a semi-crystalline thermoplastic, giving it one of the highest shrinkage ranges commonly encountered in injection moulding. As the polymer crystallises during cooling, its molecular structure becomes more tightly packed, resulting in greater contraction than amorphous plastics. For HDPE shrinkage in injection moulding, mould cavity sizing, uniform wall thickness, cooling consistency and generous draft angles are critical to minimise warpage and achieve dimensional accuracy.

ABS Shrink rate

ABS shrink rate –  .004- .008 in/in (0.4 – 0.8%). As an amorphous thermoplastic, ABS exhibits relatively low and predictable shrinkage because it does not undergo crystallisation during cooling. This makes it a popular choice for parts requiring tight tolerances and good dimensional stability. For comparison, PC/ABS blends have a slightly lower shrinkage range of .004 – .007 in/in (0.4 – 0.7%), offering even greater dimensional consistency while combining the toughness of polycarbonate with the processability of ABS.

Polypropylene shrink rate

Polypropylene (PP) shrink rate –  .010 – .030 in/in (1.0 – 3.0%). PP is a semi-crystalline resin with relatively high and variable shrinkage due to crystallisation during cooling. The final shrinkage can vary significantly depending on part geometry, wall thickness, mould temperature and cooling conditions. Designers should account for this variability early in the tool design process, using uniform wall sections and balanced cooling to reduce differential shrinkage, sink marks and warpage.

Nylon shrinkage

Nylon (Polyamide) shrinkage varies considerably depending on whether the material is reinforced. Unfilled nylon typically shrinks .007 – .025 in/in (0.7 – 2.5%), while glass-filled nylon shrinks just .005 – .010 in/in (0.5 – 1.0%). Glass fibers restrict polymer movement as the material cools, reducing overall shrinkage and making it more uniform. This improved dimensional stability is one of the primary reasons glass-filled nylon is specified for precision engineering components that require tight tolerances and reduced warpage.

How to calculate shrinkage percentage

Plastic shrinkage is typically calculated using the following formula:

Shrinkage (%) = (Mould cavity dimension − Finished part dimension) ÷ Mould cavity dimension × 100

Worked Example

If a mould cavity is 100.0 mm long and the finished moulded part measures 99.3 mm, the shrinkage is:

Shrinkage (%) = (100.0 − 99.3) ÷ 100.0 × 100 = 0.7%

This is equivalent to a shrinkage rate of .007 in/in (0.007 mm/mm).

How Toolmakers Use the Shrink Factor

Toolmakers account for material shrinkage before the mould is manufactured by cutting the mould cavity oversize. The cavity dimensions are increased by the expected shrink factor so that, after the molten plastic cools and contracts, the finished part reaches its required dimensions.

For example, if a component must measure 100.0 mm after moulding and the selected material has a shrinkage rate of 0.7% (.007 in/in), the mould cavity would be machined to approximately 100.7 mm. As the part cools and shrinks by around 0.7 mm, it produces a finished component close to the target 100.0 mm dimension. Because actual shrinkage is also influenced by part geometry, wall thickness, mould design and processing conditions, toolmakers often fine-tune cavity dimensions during tool trials to achieve the final required tolerances.

Mould shrinkage calculator

Use the calculator below to estimate the mould cavity dimension your toolmaker should machine to. Enter your part’s target dimension and select a material to see the recommended cavity size and expected shrinkage range.

Calculator that determines the mould cavity dimension a tool should be machined to, based on the target part dimension and the material’s shrink rate range

Recommended cavity size

100.4–100.8 mm

Expected shrinkage

0.4–0.8 mm

Based on typical shrink rate ranges. Confirm with your toolmaker during tool trials.


What affects the shrinkage rate?

Although every material has a typical shrinkage range, the actual amount of shrinkage depends on both the resin and the moulding process. Key factors include:

  • Mould temperature – Mould temperature has a significant influence on shrinkage. As a general guide, a 10% change in mould temperature can result in approximately a 5% change in the original shrinkage rate, particularly for semi-crystalline materials. 
  • Injection pressure – Higher injection pressure packs more material into the cavity, increasing density and generally reducing shrinkage. Lower packing pressure typically results in greater shrinkage. 
  • Resin family and fillers – Amorphous resins generally shrink less than semi-crystalline resins, while glass fiber and mineral-filled grades reduce shrinkage and improve dimensional stability compared with unfilled materials. 
  • Flow direction – Shrinkage is often different parallel to the melt flow than across the flow, especially in semi-crystalline and fiber-reinforced materials, and should be considered during tool design. 
  • Wall thickness – Thicker sections cool more slowly and tend to shrink more than thin, uniform walls, increasing the risk of sink marks and warpage. 
  • Cooling time – Consistent and adequate cooling promotes more uniform shrinkage, while uneven cooling can lead to distortion and dimensional variation. 
  • Gate location – Gate position influences material flow, packing pressure and cooling patterns, all of which affect shrinkage distribution and the likelihood of warpage across the finished part.

What is an acceptable shrinkage percentage?

There is no universal “acceptable” plastic shrinkage percentage. What is acceptable depends on the dimensional tolerance, function and performance requirements of the finished part -not the shrinkage value itself. Materials with low shrinkage, such as amorphous resins, are often selected for precision components because they are easier to mould to tight tolerances. Typical shrinkage ranges from 0.2 – 0.8%, depending on the material. In contrast, semi-crystalline resins commonly shrink 1.5 – 3.5%, but these higher values are entirely acceptable when the mould is designed with the correct shrink allowance and the process is properly controlled. The key is not achieving the lowest possible shrinkage but accurately compensating for the material’s expected shrinkage during tool design to produce parts within specification.

How Rosti compensates for shrinkage in mould design

At Rosti, plastic shrinkage is considered from the earliest stages of product development to ensure components meet their dimensional and performance requirements. Our engineering teams account for shrinkage throughout the development process in three key stages:

  • Material selection – Selecting the most appropriate polymer based on shrinkage characteristics, mechanical performance and dimensional stability. 
  • Mould flow simulation (SolidWorks) – Using mould flow analysis to predict material flow, packing, cooling and expected shrinkage before tooling is manufactured, helping to reduce development risk and optimise part quality. 
  • Tool design and validation – Applying the correct shrink factors when designing and machining the mould cavity, then validating dimensions during tool trials to achieve the required tolerances. 

Learn more about our Material Selection, Mould Flow Simulation (SolidWorks) and Tool Design & Validation capabilities to see how we engineer high-quality injection moulded components from concept through production.

If you’re developing a new injection moulded component or selecting the right material for your application, contact Rosti’s engineering team to discuss your design, tooling and manufacturing requirements.